| TPUA-250A | Caprolactone | 105~115 | 30 | 67 | 20/150 OC | 85 |
| TPUA-250B | Caprolactone | 120~130 | 8 | 77 | 20/150 OC | 100 |
| TPUA-250C | Caprolactone | 115~125 | 15 | 72 | 10/150 OC | 95 |
| TPUA-251A | Polyester | 115~125 | 10 | 70 | 40/150 OC | 95 |
| TPUA-252A | Polyester | 125~135 | 2 | 75 | 25/150 OC | 105 |
| TPUA-256A | Polyester | 110~130 | 30 | 75 | 20/150 OC | 90 |
| TPUA-256AH | Polyester | 130~150 | 35 | 75 | 2~6/150 OC | 105 |
| TPUA-257B | Polyester | 130~140 | 20 | 80 | 4/150 OC | 110 |
| TPUA-259B | Polyester | 130~140 | 6 | 90 | 30/150 OC | 110 |
| TPUA-262A | Polyester | 100~110 | 15 | 95 | 10/150 OC | 80 |
| TPUA-262H | Polyester | 125~140 | 30 | 96 | 2/150 OC | 80 |
| TPUA-263D | Caprolactone | 125~140 | 10 | 96 | 4/150 OC | 90 |
| TPUA-264A | Caprolactone | 80~90 | 4 | 98 | 10/150 OC | 59 |
| TPUA-265A | Polyester | 80~90 | 6 | 97 | 10/150 OC | 60 |
| TPUA-265AL | Polyester | 130~140 | 6 | 97 | 20~30/150 OC | 60 |
| TPUA-266A | Polyester | 90~100 | 6 | 97 | 10/150 OC | 70 |
| TPUA-266B | Polyester | 100~120 | 5 | 97 | 40/150 OC | 65 |
| TPUA-267A | Polyester | 110~130 | 6 | 97 | 10/150 OC | 90 |
| TPUA-270B | Polyether | 130~140 | 2 | 70 | 15/150 OC | 110 |
| TPUA-285AL | Polyester | 130~140 | 3 | 98 | 15~25/150 OC | 60 |
|